Stainless hlau qib 2205 - Duplex High Strength Qib
Feb 05, 2026
Tso lus



Kev sib xyaw
Table 1 muab cov kev sib xyaw ua ke rau qib 2205 duplex stainless hlau.
Table 1- Kev sib xyaw ua ke rau 2205 qib stainless hlau
|
Qib |
C |
Mn |
Si |
P |
S |
Cr |
Mo |
Ni |
N |
|
|
2205 (S31803) |
Min Max |
- 0.030 |
- 2.00 |
- 1.00 |
- 0.030 |
- 0.020 |
21.0 23.0 |
2.5 3.5 |
4.5 6.5 |
0.08 0.20 |
|
2205 (S32205) |
Min Max |
- 0.030 |
- 2.00 |
- 1.00 |
- 0.030 |
- 0.020 |
22.0 23.0 |
3.0 3.5 |
4.5 6.5 |
0.14 0.20 |
Mechanical Properties
Cov khoom siv kho tshuab raug ntawm qib 2205 stainless hlau tau teev nyob rau hauv cov lus hauv qab no. Qib S31803 muaj cov khoom zoo sib xws rau S32205.
Rooj 2- Cov yam ntxwv ntawm 2205 qib stainless hlau
|
Qib |
Tensile Str |
Yield zog |
Elongation |
Hardness |
|
|
Rockwell C (HR C) |
Brinell (HB) |
||||
|
2205 |
621 |
448 |
25 |
31 max |
293 max ua |
Xa kev nug