Stainless hlau 321

Dec 04, 2025

Tso lus

Stainless hlau 321 yog titanium-stabilized austenitic alloy, zoo ib yam li 304 tab sis nrog Ti (5 × C–0.70%). Nws tiv thaiv intergranular corrosion ntawm 425-815 degree, zoo tagnrho rau welded lossis siab - cov khoom siv cua sov xav tau kev tiv thaiv corrosion.

info-750-750

Tshuaj muaj pes tsawg leeg (Key, % ASTM A240)

C: Tsawg dua lossis sib npaug rau 0.08; Cr: 17.0–19.0; NPE: 9.0–12.0

Tis: 5 × C – 0.70 (min 0.10)

Mechanical Properties (Annealed)

Tensile Strength: Ntau dua lossis sib npaug ntawm 515 MPa; Yield zog: Ntau dua los yog sib npaug rau 205 MPa

Elongation: Ntau dua lossis sib npaug li 40%; Hardness: Tsawg dua los yog sib npaug rau 217 HB

info-750-750

Kev ua tau zoo & Kev siv

Qhov zoo: Resistant intergranular corrosion, weldable yam tsis muaj ncej- kho, ua haujlwm ntawm 870℃.

Daim ntawv thov: Aircraft exhausts, heat exchangers, boiler parts, food ncu.

Qib sib npaug

EN 1.4541, JIS SUS321, DIN X6CrNiTi18-10

info-750-750

Q&As

Ti stabilize nws li cas?Ti binds carbon ua ntej nws tsim Cr carbides (uas deplete Cr thiab ua rau corrosion). Txawm tias nyob rau hauv welded tshav kub zones, Ti xauv cov pa roj carbon, ua kom Cr sib npaug sib npaug - tsis muaj weld lwj (tsis zoo li 304).

Piv rau 316 Ti?316Ti muaj Mo (2–3%) rau cov tshuaj tiv thaiv chloride (kev siv marine) thiab ntau dua Ni (10–14%). 321 tsis muaj Mo (qhov phem dua hauv dej ntsev) tab sis pheej yig dua. Xaiv 321 rau qhuav kub kub (exhausts); 316Ti rau chlorides.

Cryogenic siv?Yog lawm. Austenitic qauv nyob qis qis qis dua -196℃(kua nitrogen). Ti tsis ua mob rau qis -temp kev ua haujlwm- khaws ntau dua lossis sib npaug li 40% elongation. Zoo rau foob pob hluav taws roj tso tsheb hlau luam, tab sis 304 yog pheej yig dua rau kev siv cryo ntshiab.

Dab tsi yog weld decay?Nws yog intergranular corrosion nyob rau hauv welded 304: tshav kub aav tsim Cr carbides, corroding yooj yim. 321's Ti tiv thaiv qhov no -welds nyob corrosion-resistant, tsis muaj ncej-weld annealing xav tau.

Cov tswv yim kho cua sov?Anneal at 925–1100°C (30–60 mins/25mm thickness) to soften and form Ti carbides. Quench in water (slow cooling causes Cr carbides). Avoid overheating >1100℃(dissolves Ti carbides).

Xa kev nug