Chemcial Composition ntawm Qib 310/310S Stainless Hlau
Cov tshuaj muaj pes tsawg leeg ntawm qib 310 thiab qib 310S stainless hlau tau sau tseg hauv cov lus hauv qab no.
Table 1.Cov tshuaj muaj pes tsawg leeg% ntawm qib 310 thiab 310S stainless hlau
|
Tshuaj muaj pes tsawg leeg |
310 |
310S |
|
Cov pa roj carbon |
0.25 max |
0.08 max |
|
Manganese |
max 2.00 Nws |
max 2.00 Nws |
|
Silicon |
1.50 max |
1.50 max |
|
Phosphorus |
0.045 max |
0.045 max |
|
Sulfur |
0.030 max |
0.030 max |
|
Chromium |
24.00 - 26.00 |
24.00 - 26.00 |
|
Nickel |
19.00 - 22.00 |
19.00 - 22.00 |
Mechanical Properties ntawm Qib 310/310S Stainless Hlau
Cov khoom siv kho tshuab ntawm qib 310 thiab qib 310S stainless hlau tau sau tseg hauv cov lus hauv qab no.
Rooj 2.Mechanical zog ntawm qib 310/310S stainless hlau
|
Mechanical Properties |
310/ 310S |
|
Qib 0.2% Pov Thawj Stress MPa (min) |
205 |
|
Tensile zog MPa (min) |
520 |
|
Elongation% (min) |
40 |
|
Hardness (HV) (max) |
225 |
Lub cev muaj zog ntawm Ferritic Stainless hlau
Lub cev lub cev ntawm qib 310 thiab qib 310S stainless hlau tau sau tseg hauv cov lus hauv qab no.
Table 3.Lub cev muaj zog ntawm qib 310/310S stainless hlau
|
Cov khoom |
ntawm |
Tus nqi |
Chav tsev |
|
Qhov ntom |
|
8,000 |
Kg / m3 |
|
Hluav taws xob conductivity |
25 degree |
1.25 |
% IACS |
|
Hluav taws xob Resistivity |
25 degree |
0.78 |
Micro ohm |
|
Modulus ntawm Elasticity |
20 degree |
200 |
GPa |
|
Shear Modulus |
20 degree |
77 |
GPa |
|
Poisson tus ratio |
20 degree |
0.30 |
|
|
Melting Rnage |
|
1400-1450 |
degree |
|
Tshwj xeeb kub |
|
500 |
J/kg. degree |
|
Sib Nqus Sib Nqus Permeability |
|
1.02 |
|
|
Thermal conductivity |
100 degree |
14.2 |
W/m. degree |
|
Coefficient ntawm Expansion |
0-100 degree |
15.9 |
/ degree |
|
|
0-315 degree |
16.2 |
/ degree |
|
|
0-540 degree |
17.0 |
/ degree |